ESAB offers a complete line of welding and cutting products and solutions. Explore our equipment offering with ease based on product line and industry.
ESAB is a world leader in welding and cutting equipment and consumables. Explore our complete line of welding & cutting products for virtually every application.
ESAB University is your online learning destination for welding and fabrication technology. Make personalized playlists of your favorite resources including videos, blogs, articles, webinars and more.
ESAB Courses are structured learning paths designed to take your welding knowledge and skills to the next level.
Articles cover industry topics more in-depth and are created in partnership with ESAB engineers and master welders. Click the links to see the latest.
ESAB blogs include information and tips from ESAB Experts to improve your welding and fabrication knowledge.
ESAB University videos are curated with tips and best practices from top fabricators around the world. Learn new techniques or improve your current skills with ESAB University videos.
Enhance your knowledge of welding, cutting, and fabrication with free and accessible webinars on a variety of topics, including welding best practices, tips for using ESAB products, new product launches, and more, presented by trusted ESAB experts.
ESAB's Future for Fabricators platform is committed to highlighting those who lead education for aspiring future fabricators. We aim to share inspirational stories, facilitate initiatives to bring tools and expertise to communities and make our equipment accessible to ensure future fabricators are set up for success - right from the start.
ESAB is a world leader in welding and cutting equipment and consumables. We offer a complete line of fabrication solutions for virtually every application.
ESAB Newsroom - Stay up to date with the latest news from ESAB. View press releases, product announcements, corporate news, and more here.
ESAB EHS (Environment, Health & Safety) initiatives are monitored with the highest degree of importance and commitment to safety is ingrained in our culture.
The history of ESAB is the History of Welding. Go here to view an interactive look at ESAB's history in shaping the future of innovation in welding, cutting, and fabrication.
View available job openings and more on the ESAB Careers page.
ESAB offers a wealth of product support resources, including a range of technical and service publications, from Safety Data Sheets and downloadable product manuals to product certifications.
Visit ESAB's global manual search engine to access the items below and more.
Global User Manuals
Instruction Manuals
Spare Parts List
Product Storage Instructions
View Main Contact Page
View ESAB Location Information
No playlist found! Your playlist can be created here.
Weld porosity results from the entrapment of hydrogen gas. This gas entrapment results in lower weld strength and ductility by reducing the crosssectional area of sound metal and by acting as stress risers which cause premature failure. Several variables can produce gas porosity, one of which is the surface condition of the aluminum filler wire. The qualities relating to the surface characteristics of the filler wire include:
Of these three surface conditions, the most common cause of weld porosity is the presence of hydrocarbons. Examples of these compounds include residual wire drawing lubricants, mill dirt or even fingerprints. One relatively quick and inexpensive method of testing aluminum welding wire for freedom from residual hydrocarbons is by means of a “Smoke Test".
The “Smoke Test" is a qualitative test performed by heating a sample of wire using an electrical resistance heating machine. While conducting the test, the wire is visually examined for the presence of smoke, caused by the burning of any surface contamination. Minute amounts of contamination, even a fingerprint, will result in smoke. The schematic shows a typical smoke tester machine(1) . Just about any commercial welding power source will suffice. The weld cables are connected to two hobby vises. The wire sample completes the circuit. A light with a dark viewing background is recommended to aid in observing any smoke as the test is performed. Care must be taken in selecting and placing the sample in the vise grips so that the wire does not come in contact with any contamination, including human hands.
CAUTION: Do not touch the wire after testing since it becomes extremely hot.
The schematic also details typical amperage settings based upon the alloy and diameter of the sample to be tested. The amperage is chosen to control the melt rate of the sample and allow adequate time to detect the presence of any smoke. The amperage should be sufficient to melt the sample in 3 to 5 seconds.
SUGGESTED AMPERAGE SETTINGS BY ALLOY SERIES 1XXX Sizes 2XXX 4XXX 5XXX .030 45 40 40 .035 50 50 50 .040 60 60 60 .047 90 90 70 .062 140 120 120 .094 225 225 225
A direct correlation exists between smoke test results and weld porosity. Zero smoke should indicate minimal weld porosity. A small amount of smoke will indicate some evidence of weld porosity generated by contamination. A large amount of smoke will indicate severe contamination and the filler wire should be further examined before continuing production welding.
Design, technical reference charts and other information presented herein have been researched for accuracy, however, are given without expressed or implied warranty, guarantee or responsibility of any kind on the part of AlcoTec.
The "Twist Test" can be conducted on spooled or straight-length wire to show the presence of surface imperfections. It can also be done on an electrode that has passed through the welding equipment. A sample taken after going through the welding gun may show abrasion from drive rolls, guides, or the contact tip. The abrasions create fines, which in turn plug the liner and contact tip, and create burnbacks.
To check the wire for surface abrasions, take a 10-inch sample and put a 90° bend 2 inches from each end. Twist one end 5 or 6 times afull 360°.
The surface of the twisted sample should stay smooth. Check for lines by dragging a fingernail down the length of the twisted portion. Metallic fines (aluminum dust) may also be present if the wire surface has been disturbed. AlcoTec routinely conducts twist tests on wire to ensure surface smoothness and freedom from surface imperfections.